In short
- In Turkish Standards Institution tests, 10 % citric acid, 5 % acetic acid, 25 % caustic soda and 30 % hydrogen peroxide left no visible change on any of five HPL constructions.
- Ink is the hard case: it marked a standard laminate (grade 2), while an aluminium oxide overlay lifted the result to grade 5.
- Rushil's TOPAZ and VAULT compact report grade 5 in all three EN 438 staining groups, including group 3, where the standard accepts 4.

How this review was put together
This article summarises three peer-reviewed laboratory studies: a comparison of HPL layer structures from Gazi University and Karadeniz Technical University, tested in the laboratories of the Turkish Standards Institution (Burdurlu and Özgenç, Forest Products Journal, 2009); a study of antimicrobial HPL from the University of Aveiro (Magina et al., Materials, 2016); and work on modified melamine resin from Qingdao (Chen et al., RSC Advances, 2019). It sets Rushil's published staining results beside them. All three studies tested laboratory samples; the papers are listed at the end.
Acids, alkalis and oxidisers
Burdurlu and Özgenç put five laminate constructions through staining tests to EN 438 with four chemicals: 10 % citric acid, 5 % acetic acid, 25 % sodium hydroxide, the active ingredient of caustic soda, and 30 % hydrogen peroxide. Every construction scored grade 5, the top of the scale, for every chemical: no visible change at all.
Those concentrations go well beyond everyday cleaning products. That the melamine surface shrugged off a strong alkali and a strong oxidiser alike is the clearest evidence in the study of why HPL is chosen for kitchens, laboratories and hospitals.
Ink is the hard case
One agent did tell the constructions apart. Ink left a mark on the standard laminate, graded 2, and on those with a barrier layer, graded 3. An overlay lifted the result to 4, and a barrier with an aluminium oxide overlay to 5, no visible change. The same layer raised the laminate's wear resistance about 35 times and its resistance to cigarette burns from grade 2 to 5, as other articles on this site explain.
What EN 438 asks, and what research adds
EN 438-2 sorts its staining agents into three groups. Rushil's data sheets give the requirements: for groups 1 and 2 no visible change at all, grade 5; for group 3 at most a slight change, grade 4. The antimicrobial HPL developed in Aveiro scored grade 5 in all three groups, against the required 4 the authors cite, while its additive also stopped bacterial growth.
Research keeps raising the bar. In Qingdao, researchers modified the melamine resin of HPL with polyvinyl alcohol and benzoguanamine and left hot coffee and ink on it for 24 hours. The standard laminate kept stains, the modified one showed no obvious change. It is a laboratory development, but it shows where the next generation of surfaces is heading.
What Rushil's data sheets report
Rushil's TOPAZ and VAULT compact data sheets report grade 5 for staining in all three EN 438 groups, including group 3, where the standard would accept 4. The Decorative HPL data sheet reports grade 5 for groups 1 and 2 and grade 4 for group 3, the required level. These are test results, not a declaration of conformity.
What this means for kitchens, labs and hospitals
The studies agree on the essentials. The melamine surface of HPL resisted acids, a strong alkali and a strong oxidiser without any visible change; ink is the stubborn case, and an aluminium oxide overlay answers it. For a surface that meets coffee, wine, cleaners and disinfectants every day, that is the property that keeps it looking new.
For worktops and serving counters, TOPAZ brings grade 5 in every staining group on a solid compact core; for washrooms, cubicles and hospital walls, VAULT does the same. Follow the cleaning guidance on this site, avoid scouring pads that scratch, and ask for samples to test with your own products.
Common questions
Will coffee or wine stain an HPL worktop?
Everyday drinks belong to the agents of the EN 438 staining test. Rushil's TOPAZ data sheet reports grade 5, no visible change, in all three staining groups. Wipe spills promptly all the same; research shows that dark agents such as ink are the hardest case.
Can HPL be cleaned with strong chemicals?
In the Turkish Standards Institution tests, 25 % sodium hydroxide and 30 % hydrogen peroxide left no visible mark on any of five HPL constructions. Follow the maker's cleaning guidance and avoid abrasive pads, which can scratch even a chemically resistant surface.
Why does an aluminium oxide overlay matter for stains?
In the same tests it lifted ink resistance from grade 2 on the standard laminate to grade 5, as well as multiplying wear resistance and improving resistance to cigarette burns.
Sources
- Forest Products Journal 59(4), Burdurlu E., Özgenç Ö. — Effect of different layer structures on some resistance characteristics of high-pressure laminatesApr 1, 2009 · en
- Materials 9(2), Magina S., Santos M. D., Ferra J., Cruz P. et al. — High Pressure Laminates with Antimicrobial PropertiesFeb 6, 2016 · en
- RSC Advances 9(63), Chen X., Afreen S., Yu X., Dong C., Kong Q. — Modified melamine-formaldehyde resins improve tensile strength along with antifouling and flame retardancy in impregnation of cellulose paperJan 1, 2019 · en
- Rushil Decor — VIR TOPAZ (CGS / CGF) — Product Data Sheeten
- Rushil Decor — Decorative HPL (HGS/VGS) — Product Data Sheeten
Compiled for this site from the publications listed above. Summaries are in our own words, not quotations — read the originals for the full argument.